Filament Drying & Storage
Filament Drying & Storage
Section titled “Filament Drying & Storage”Most 3D printing filaments absorb moisture from the air. In the hot end that water turns to steam, so the molten plastic bubbles and extrudes unevenly. The results are stringing, oozing, pitted or rough surfaces and weaker parts. How much this matters depends on the material and on your climate.
This page combines discussions from the IrregularChat Fabrication chat (December 2025 to October 2026) with manufacturer drying guidance. Members are not named.
Do I Need a Dryer?
Section titled “Do I Need a Dryer?”The chat’s answer: if you print anything other than PLA or PETG, or you live somewhere humid, yes.
- TPU, nylon (PA), PC, PVA and wood-fill PLA: drying is required. Wet TPU strings badly. Wood-fill PLA “holds moisture” and “needs to dry a lot”, so plan for it.
- PLA and PETG for functional parts: often fine without drying in a dry climate. A member who used to live in Colorado never needed to dry anything there. Members in North Carolina, Georgia and Missouri dry everything, PLA included. Florida: yes. Texas: usually not.
- New spools: one member dries every spool, including new ones straight out of the packaging. Factory sealing doesn’t help if the spool sat open before it reached you (see the cautionary tale below).
What moisture does to prints, in one member’s words: “stringy in the near term, and pimply in the long term.”
Signs of Wet Filament
Section titled “Signs of Wet Filament”- Popping, crackling or hissing at the nozzle, sometimes with visible steam
- Stringing and oozing that wasn’t there with the same settings before
- Bubbles, pits or a “pimply” or rough surface
- Brittle filament that snaps in the feed path (old PLA especially)
- Weak layers and poor bridging
Dryer Options the Community Uses
Section titled “Dryer Options the Community Uses”These are products members have used or recommended, as of October 2026. Maximum temperatures come from the manufacturer or retailer listings.
| Dryer | Type | Max temp | Community notes |
|---|---|---|---|
| SUNLU AMS Heater | Heated lid for the Bambu Lab AMS (Gen 1) | 70 °C | The most-recommended option in the October 2026 thread. Members use it on a P1S, can dry while printing from the AMS, and one member in Missouri leaves it running constantly because of the humidity. |
| Bambu Lab AMS 2 Pro | AMS with built-in drying | 65 °C | Members said it won’t dry and print at the same time. Bambu’s wiki now describes drying during a print at a reduced temperature (see below), so check your firmware. Not suitable for ABS, ASA, PC or nylon. On an X1 or P1 printer, each unit needs its own power adapter to dry. |
| Bambu Lab AMS HT | Single-spool, high-temperature AMS | 85 °C in Bambu’s table | Can dry every material Bambu lists except PPA-CF and PPS-CF; PVA may not fully dry. Needs its own power cable. |
| Sovol SH01 | 2-spool dry box | 50 °C (listed range 40–50 °C) | “That one is nice but doesn’t get above 50 so harder for ABS.” Fine for PLA, marginal for PETG, not enough for ABS, ASA, PC or nylon. |
| Creality SpacePi X4 | 4-spool, 2-chamber dryer | 85 °C (one retailer lists 80 °C) | One member chains it to a Prusa MMU3 on a Core One so the spools stay heated and enclosed. The MMU3 itself leaves filament in open air, and its rollers can bind on cardboard spools. |
| Printer heated bed | Built-in, enclosed printers only | Bed temperature | Bambu supports this on enclosed printers: cover the spool with its cardboard box or a printed PC cover and flip it halfway through. On a P1S you set the bed temperature and keep time yourself. Open-frame printers (A1, A1 mini, P1P) can’t do this. |
Drying while printing
Section titled “Drying while printing”Two questions came up in the chat.
Can I dry and print at the same time?
- SUNLU AMS Heater: yes. It heats the whole AMS while the AMS feeds the printer.
- Bambu AMS 2 Pro and AMS HT: Bambu’s store FAQ says drying is blocked for any unit that is part of the print. Bambu’s own wiki (checked 2026-10-22) now says that once a print starts, the drying temperature drops below the filament’s softening point instead: 45 °C when drying PLA or printing with PLA, 55 °C when drying PETG while printing ABS or PETG. It also says the AMS won’t dry while auto-feed is running, so the gears don’t deform softened filament. Treat drying during a print as reduced and firmware-dependent.
- A member pointed out the trade-off: different materials dry at different temperatures, so one heater shared by four mixed spools is always a compromise.
If the filament is already dry, does heating it during the print help? Mostly no, as long as it stays sealed. One member in humid Georgia dries ABS first and then prints it unheated with no problems. What matters is the humidity around the spool while it prints:
- At about 20% relative humidity (RH), dried filament generally stays dry for 2 to 7 days.
- In a typical room at about 55% RH, freshly dried filament absorbs enough water to hurt print quality within 2 to 12 hours.
So in a humid area, either keep the spool in a sealed AMS or box with fresh desiccant, or keep a heater running during long prints.
Drying Temperatures by Material
Section titled “Drying Temperatures by Material”These figures are from Bambu Lab’s Filament Drying Recommendations (Appendix I, checked 2026-10-22). They were written for Bambu filaments. For other brands, use the manufacturer’s numbers if they publish them, and stay below the spool’s heat limit.
| Material | Dry before use? | Forced-air dryer / oven | Heated bed (enclosed, covered) | AMS 2 Pro | AMS HT |
|---|---|---|---|---|---|
| PLA Basic / Matte | Recommended | 50 °C, 8 h | 60–70 °C, 12 h | 45 °C, 12 h | 45 °C, 12 h |
| PLA Silk / Galaxy | Recommended | 55 °C, 8 h | 65–75 °C, 12 h | 45 °C, 12 h | 45 °C, 12 h |
| PLA-CF / GF | Recommended | 50–60 °C, 8 h | 65–75 °C, 12 h | 45 °C, 12 h | 45 °C, 12 h |
| PLA Wood | Required | 55–65 °C, 8 h | 70–75 °C, 12 h | 45 °C, 12 h | 45 °C, 12 h |
| PETG, PETG-CF | Recommended | 60–65 °C, 8 h | 75–85 °C, 12 h | 65 °C, 12 h | 65 °C, 12 h |
| ABS, ASA | Recommended | 75–85 °C, 8 h | 90–100 °C, 12 h | Not compatible | 80 °C, 8 h |
| TPU 85A–95A | Required | 70 °C, 8 h | 80–90 °C, 12 h (85A/90A: 90 °C, 16 h) | 65 °C, 12 h (may not fully dry) | 75 °C, 18 h |
| PC | Required | 75–85 °C, 8 h | 90–100 °C, 12 h | Not compatible | 80 °C, 8 h |
| PVA | Required | 75–85 °C, 8–12 h | 90–100 °C, 12 h | Not compatible | 85 °C, 18 h |
| PA6-CF/GF, PAHT-CF/GF (nylon) | Required | 75–85 °C, 8–12 h | 90–100 °C, 12 h | Not compatible | 85 °C, 12 h |
| PET-CF | Required | 80 °C, 8–12 h | 90–100 °C, 12 h | Not compatible | 80 °C, 12 h |
| PPA-CF, PPS-CF | Required | 100–140 °C, 8–12 h | 110–120 °C max, 10–12 h (less effective) | Not compatible | Not compatible |
- Don’t use a kitchen oven or a microwave. Kitchen ovens have hot spots near the elements that can melt spools. Microwaves heat unevenly and can’t hold a temperature. Use a forced-air (convection) dryer or oven with the spool away from the heating element.
- Don’t exceed the spool’s heat limit. Cardboard and some third-party plastic spools deform. Re-spool them onto a reusable spool first (members print re-spoolers for this).
- Don’t re-dry PC over and over. Repeated heating and cooling makes PC filament brittle and more likely to snap in the feed path, even though printed parts aren’t weaker. Keep it sealed after drying so it needs little or no re-drying.
Storage
Section titled “Storage”Drying only helps if the filament stays dry afterwards.
- Seal it with desiccant right after drying: an AMS with fresh desiccant, a sealed bin or a vacuum bag. Put a cheap hygrometer in each box so you can see the humidity.
- Aim for below 20% RH. Typical indoor air is 45–65% RH.
- Replace or regenerate desiccant when the hygrometer creeps up.
- For a large collection, members have looked at electronic dry cabinets (humidity cabinets), the kind used for camera gear and electronics, instead of many separate bins.
- Long-term stock (nylon, PC, PVA, TPU) stays in its original sealed bag with desiccant until you need it. Don’t let anyone unpack a pallet and leave the spools open.
Related Pages
Section titled “Related Pages”- Fabrication - Main fabrication hub and community files
- 3D Printer Recommendation - Choosing a printer, including enclosure and AMS considerations
- Getting Started with CAD - CAD software for designing parts
- Unmanned Systems - sUAS builds that rely on TPU, nylon and CF parts
References
Section titled “References”- Bambu Lab Wiki: Filament Drying Recommendations - Drying table, AMS 2 Pro and AMS HT notes, storage humidity guidance
- Bambu Lab AMS 2 Pro (store page and FAQ) - Drying and power requirements
- Bambu Lab Wiki: Filament Drying Cover - Printable cover for heated-bed drying